Reactive Stain Instructions
The wood must be clean, dry and free from dust.
Sanding
Final sanding grit 120-150
Spray
40-60 gr/m2 Or use sponge roller
Roller
Use sponge roller shore 5 or type 2 or type 3 Apply the product 30-35 gr/m2
Even out
Use minimum two nylon brushes. 1st runs counterwise and 2nd runs counter-clockwise
Hot air oven
Temperature 50-60 °C and good ventilation Or use stacking on racks
Stacking
3-4 h by 20 °C
Intermediate sanding
Use sand paper grit 240-320 After sanding apply a WOCA Treat product
Viscosity correction: Not recommended. If the color is too dark, water can be added to achieve the right design.